Optical Properties | Value |
---|---|
Refractive index* nd for cover glass (as drawn) | 1.5080 ± 0.003 |
Total normal emittance εn of cover glass top surface at 25 °C |
≤ 0.86 |
Thermal properties | Unit | Value |
---|---|---|
Transformation temperature Tg
|
in °C | 568 |
CTE (coefficient of thermal expansion) α | in 10-6 · K-1 (20 °C; 300 °C) |
8.5 |
in 10-6 · K-1 (20 °C; 150 °C) | 7.9 |
Mechanical Properties |
Unit | Value |
---|---|---|
Density ρ | in g/cm³ | 2.51 ± 0.05 |
Young's modulus E | in kN/mm² | 70.0 |
Poisson's ratio µ | 0.216 | |
Breaking strength | Strength-optimized cutting process, details available on request |
Electrical properties | Value |
---|---|
Bulk resistivity ρD | > 1 ∙ 1011 Ω m (ν = 20 °C) |
Reference values of typical production quality
Transmittance values
Spectral transmittance
Technical Details - Solar Glass sphere
Optical Properties | Unit | Value |
---|---|---|
Refractive index* nd | 1.5231 | |
Edge wavelength λc (τ = 0.46) | in nm (thickness in mm) |
308 |
Luminous Transmittance 𝛕vD65 | in nm (thickness in mm) |
91.8 (0.1) |
Thermal properties | Unit | Value |
---|---|---|
Transformation temperature Tg | in °C | 557 |
CTE (coefficient of thermal expansion) α | in 10-6 · K-1 (20 °C; 300 °C) | 7.2 |
Mechanical Properties |
Unit | Value |
---|---|---|
Density ρ | in g/cm³ | 2.51 |
Young's modulus E | in kN/mm² | 72.9 |
Poisson's ratio µ | 0.21 | |
Breaking strength | Strength-optimized cutting process, details available on request |
SCHOTT® Solar Cell Cover Glasses are available as:
- Sheets
- Cut-to-size substrates
- Unpolished substrates and wafers
To find out more, please see the related products on the overview page.
Preview environment - pls. be aware that this page only displays the staged content and is not functional!